Foundation & Structure · How-to Guide

Slump Test for Concrete: Procedure, Readings and Interpretation

How to run the slump cone test exactly as IS 1199 (Part 2):2018 sets it out, read true, shear and collapse slump, and judge a reading against the ordered value on site.

On this page
  1. What Is the Slump Test of Concrete and Why Does It Matter?
  2. What Apparatus Does IS 1199 (Part 2):2018 Specify?
  3. How Do You Do the Slump Test of Concrete, Step by Step?
  4. What Do True, Shear and Collapse Slump Tell You?
  5. How Do You Interpret Slump Test Results on Site?
  6. What Mistakes Make Slump Test Readings Wrong?
  7. When Is the Slump Test of Concrete Not the Right Test?
  8. How Often Should You Test Slump on a Building Site?
0%
Summary — what you need to know
  • The slump test of concrete measures the consistency of fresh concrete, a quick proxy for workability.
  • In India, follow IS 1199 (Part 2):2018: 3 layers, 25 strokes each, lift the cone in 5 ± 2 s.
  • Only a true slump counts. A shear or collapse means a fresh sample and a repeat test.
  • Start the test within 5 minutes of taking the sample, and finish filling to lifting within 180 s.
  • For ready-mixed concrete, compare the reading with the ordered slump using the IS 4926:2003 tolerance.

The slump test of concrete is a field test that measures how much a cone of fresh concrete settles after the mould is lifted. The drop, in millimetres, tells you the consistency of the batch before it goes into the formwork.

This guide focuses on doing the test right and reading the result. For the slump each type of work needs, see our slump value of concrete guide.

300 mm
Height of the standard slump cone, IS 1199 (Part 2):2018
3 × 25
Layers × tamping strokes per layer
180 s
Maximum time from start of filling to lifting the cone

What Is the Slump Test of Concrete and Why Does It Matter?

The slump test of concrete is the standard site check of fresh concrete consistency. Consistency means how wet or stiff the mix is, and it is the part of workability the slump cone can see.

Workability is the ease of mixing, placing, compacting and finishing concrete without segregation. Segregation is when stone separates from the mortar.

The test matters because it catches batch-to-batch changes in minutes. A sudden jump in slump usually means extra water. Extra water raises the water-cement ratio and lowers strength.

  • Quality control: every batch can be checked at the point of pour.
  • Acceptance: ready-mixed concrete (RMC) is accepted or rejected on slump at discharge.
  • Low cost: the kit is a metal cone, a rod, a base plate and a ruler.
  • Speed: one test takes under 5 minutes from sampling to reading.
Insight: slump measures consistency, not strength

Two mixes with the same slump can have very different strengths. A mix made wet with water and one made flowing with a superplasticiser may both read 100 mm. Only the water-cement ratio and cube tests tell you about strength. Our water-cement ratio guide explains the link.

What Apparatus Does IS 1199 (Part 2):2018 Specify?

IS 1199 (Part 2):2018 specifies a metal slump cone, a steel tamping rod, a flat base plate, a ruler and a timer. IS 1199 is the Bureau of Indian Standards (BIS) code for sampling and testing fresh concrete, and Part 2 covers consistency.

Slump test apparatus, IS 1199 (Part 2):2018 Clause 4.3.2

Dimensions with tolerances
ItemRequirementCheck
Slump cone (mould)Metal, at least 1.6 mm thick; base 200 ± 2 mm, top 100 ± 2 mm, height 300 ± 2 mmCalibrate once a year
Tamping rodSteel, 16 ± 1 mm diameter, 600 ± 5 mm long, rounded endsOnce a year
Base plateRigid, flat, smooth and non-absorbentLevel before every test
RuleGraduated 0 to 300 mm, intervals of 5 mm or lessReadable markings
TimerAccurate to 1 sPhone stopwatch is fine
Source: IS 1199 (Part 2):2018. You also need a scoop, a shovel, a non-absorbent mixing tray and a damp cloth.

Pre-test readiness checklist

  • Cone, rod and base plate are clean, with no hardened concrete inside the cone.
  • Cone interior and base plate are damp but free of standing water.
  • Base plate sits on firm ground, away from mixer or vibrator vibration.
  • Rule and timer are within reach before sampling starts.
  • The ordered slump and tolerance are written on the delivery ticket or pour card.
  • Gloves, boots and eye protection are on: wet cement is alkaline and burns skin.

How Do You Do the Slump Test of Concrete, Step by Step?

You do the slump test of concrete by filling a cone in three tamped layers, lifting it straight up and measuring the drop. The steps below follow IS 1199 (Part 2):2018, with sampling from IS 1199 (Part 1):2018.

How should you sample the concrete?

Take a composite sample, meaning several scoops mixed together, not a single scoop. From a truck mixer, IS 1199 (Part 1) says to skip the first and last 10 to 15% of the discharge.

  • Increments: take scoops from at least four points in the discharge.
  • Avoid segregated parts: never scoop from a pile where stone has rolled away from mortar.
  • Remix: turn the sample over on a non-absorbent tray before testing.
  • Protect it: shade the sample from sun, wind and rain.

What are the slump test procedure steps?

  1. Set up: place the damp cone on the damp, level base plate. Stand on the foot pieces to hold it down.
  2. Fill layer 1: fill to about one-third of the cone height and give it 25 strokes with the rounded end of the rod, spread over the whole area.
  3. Fill layer 2: fill to about two-thirds and give 25 strokes. The rod should just enter the layer below.
  4. Fill layer 3: overfill the top and give 25 strokes. Add concrete if the level drops below the rim while tamping.
  5. Strike off: level the top with a rolling motion of the rod and clear spilled concrete from the base plate.
  6. Lift the cone: raise it straight up in 5 ± 2 s with no twisting or sideways movement.
  7. Measure: set the empty cone beside the concrete, lay the rod across its top and measure down to the highest point of the slumped concrete.
  8. Record: note the slump to the nearest 5 mm and the slump shape: true, shear or collapse.
Slump test steps as per IS 1199 Part 2: set up the cone, fill three layers with 25 strokes each, strike off, lift in 5 seconds, measure slump as 300 mm minus height, with true, shear and collapse slump shapes

How long should each stage take?

The whole test runs on a clock. IS 1199 (Part 1) says to start slump testing within 5 minutes of collecting the last part of the sample.

0 min

Sample complete

Last increment taken from the discharge; remix on the tray.

Within 5 min

Start filling

Begin the first layer. Start the timer.

Within 180 s

Cone lifted

Filling, tamping, striking off and the 5 ± 2 s lift, done without a break.

Immediately

Read and record

Measure the drop, note the shape, write it on the pour record.

How is the slump value calculated?

Slump is the cone height minus the height of the highest point of the slumped concrete. Measuring down from the rod laid on the inverted cone gives the same number directly.

The formula
Slump h = 300 mm − H
H = height of the highest point of the slumped concrete above the base plate, in mm. Report h to the nearest 5 mm.
Worked exampleReading a slump on site
Cone height300 mm
Highest point of slumped concrete, H212 mm
Slump: 300 − 21288 mm
Round to the nearest 5 mm90 mm
ResultReport a true slump of 90 mm

What Do True, Shear and Collapse Slump Tell You?

True, shear and collapse are the three shapes concrete can take after the cone is lifted, and only a true slump gives a valid reading. The shape matters as much as the number.

Types of slump and what to do, IS 1199 (Part 2):2018 Clause 4.3.4

Shape decides validity
Slump typeWhat you seeWhat it suggestsAction
True slump ValidConcrete settles evenly and keeps a rough cone shapeCohesive, plastic mixRecord to the nearest 5 mm
Shear slump RepeatOne side shears off and slides down at an angleLack of cohesion, often a harsh or lean mix, or uneven tampingTake a new sample and repeat
Collapse slump RepeatConcrete flattens and spreads across the plateVery wet mix, or a flowing mix outside the test rangeRepeat; if flowing by design, use a slump flow test
If two tests in a row shear or collapse, IS 1199 (Part 2) says to report the test as invalid: the concrete lacks the plasticity and cohesion the slump test needs.
Insight: look at the edges, not only the height

A true slump with a ring of watery mortar running out, or bare stone at the base, still signals bleeding or segregation. Note it on the record even when the number is in range.

How Do You Interpret Slump Test Results on Site?

You interpret a slump test result by comparing the true slump with the slump specified for that pour, within the allowed tolerance. The specified value comes from the structural engineer, the mix design or the RMC order.

What slump values does IS 456 suggest?

IS 456:2000, the Indian code for plain and reinforced concrete, gives slump ranges by placing condition in Clause 7.1. The short version is below; our slump values by type of work covers the full table.

Typical slump ranges, IS 456:2000 Clause 7.1

Short reference
Placing conditionSlump (mm)
Mass concrete, lightly reinforced slabs, beams, columns25–75
Heavily reinforced slabs, beams, walls, columns Most RCC50–100
Pumped concrete, slipform work75–100
Trench fill, in-situ piling100–150
Source: IS 456:2000 Clause 7.1. Tremie concrete and very low workability mixes use other tests. Follow the slump in your drawings or mix design where one is given.

What tolerance applies to ready-mixed concrete?

IS 4926:2003, the Indian code for ready-mixed concrete, sets the slump tolerance at ±25 mm or ±one-third of the specified value, whichever is less. Compliance is judged at discharge from the truck, not at the plant.

Worked exampleAccept or reject a 100 mm order
Specified slump100 mm
One-third of specified: 100 ÷ 333.3 mm
Lesser of 25 mm and 33.3 mm±25 mm
Acceptable band: 100 − 25 to 100 + 2575–125 mm
Measured true slump (example above)90 mm
Result90 mm is inside 75–125 mm: accept the load

At a specified 75 mm, both limits give ±25 mm. Below 75 mm, the one-third rule gives a tighter band, so confirm the clause with your engineer.

What does a high or low reading usually mean?

  • Higher than ordered: water added at site or in the drum, wet sand, or the wrong mix sent.
  • Lower than ordered: slump loss from a long transit, hot weather or a fast-setting admixture.
  • Big swings between trucks: poor batching control at the plant; ask for batch records.
Rule of thumb: never fix low slump with a hose

IS 4926:2003 does not allow water beyond what the specified workability needs, and any addition must be recorded on the delivery ticket and signed by the purchaser. Ask the supplier to restore slump with admixture under the engineer's approval instead.

In Bengaluru, traffic police restrict heavy goods vehicles at peak hours, so pours are often planned around those windows and transit times vary. Test each truck at discharge. Our transit mixer guide explains drum handling between plant and site.

What Mistakes Make Slump Test Readings Wrong?

Most wrong slump readings come from poor sampling, uneven tamping, a slow or tilted lift and delays. Each one changes the number without any change in the concrete.

  • Sampling from the first or last part of the discharge, where the mix is least representative.
  • Using a dry cone or base plate, which pulls water out of the concrete and lowers slump.
  • Wet puddles inside the cone or on the plate, which raise slump.
  • Filling in one go, or using fewer or more than 25 strokes per layer.
  • Tamping only the centre of each layer, which often causes a shear slump.
  • Lifting the cone with a twist, a tilt or a jerk instead of a steady 5 ± 2 s lift.
  • Testing on a sloping or vibrating surface next to a running mixer or needle vibrator.
  • Letting the sample stand for 10 to 15 minutes before testing.
  • Using a dented cone or a rod with a sharp end.
Watch out: sun, wind and heat change the reading

Fresh concrete loses slump with time, and it loses it faster in heat, wind or direct sun. Test in shade, keep the sample covered and stick to the 5-minute start limit. Admixture mixes can lose slump quickly, so note the time of testing on every record.

When Is the Slump Test of Concrete Not the Right Test?

The slump test of concrete is not suitable for very stiff mixes, very fluid mixes or self-compacting concrete. IS 1199 (Part 2):2018 limits it to slumps from 10 mm to 210 mm.

  • Stiff mixes: below 10 mm the cone barely moves, so small differences cannot be read.
  • Flowing mixes: above 210 mm the concrete collapses and the drop stops being meaningful.
  • Large aggregate: ASTM C143 does not apply when a large share of the stone is bigger than 37.5 mm.
  • Single property: slump says little about pumpability, finishing or cohesion under vibration.

Workability tests in IS 1199 (Part 2):2018

Pick by consistency
TestBest forWhat it measures
Slump test DefaultMost site concrete, 10–210 mm slumpVertical drop of a cone
Compacting factor testLow workability mixesDensity after free fall vs full compaction
Vee-Bee consistometerVery stiff mixes, precast and pavementsSeconds of vibration to remould a cone
Flow table testHigh workability mixes (not SCC)Spread diameter after jolting
Slump flow testSelf-compacting concrete (SCC)Spread diameter with no tamping; see IS 1199 (Part 6)
Source: IS 1199 (Part 2):2018 scope. Part 2 also includes a degree of compactability test.

How does IS 1199 compare with ASTM C143?

IS 1199 (Part 2):2018 and ASTM C143, the American standard test method for slump of hydraulic-cement concrete, now follow almost the same procedure. AASHTO T119 is the highway-agency version of the ASTM method.

Slump test of concrete: IS code vs ASTM

Key procedure limits
ItemIS 1199 (Part 2):2018ASTM C143IS 1199:1959 (old)
Layers334
Strokes per layer252525
Cone lift time5 ± 2 s5 ± 2 sSlowly, at once
Fill-to-lift limit180 s2.5 minNot stated
Read toNearest 5 mmNearest 1/4 in (5 mm)Nearest 5 mm
The 1959 edition has been replaced by the 2018 parts. Lab manuals and older PDFs that say "four layers" follow the old code.
Note: slump is set at the design stage

The target slump is chosen when the mix is designed, together with the water content and admixture dose. Our concrete mix design guide shows how slump changes the water per m³.

How Often Should You Test Slump on a Building Site?

Test slump on every truck of ready-mixed concrete, and on site-mixed concrete at the start of each pour and whenever the mix looks different. IS 4926:2003 asks for random workability checks and inspection of each load before discharge.

  • Every RMC truck: test at discharge before the concrete goes into the formwork.
  • Site-mixed batches: test the first batch, then whenever sand moisture or the mix changes.
  • With every cube set: record slump for the same sample used for cubes.
  • After any delay: retest a truck that has waited on site.
  • Keep a record: date, time, truck number, location in the structure, slump, shape and tester's name.

Slump is one check among several. Cube tests at 7 and 28 days, correct curing and proper compaction decide the final quality of the structure.

60-minute delivery

Mixing concrete on site?

Cement, sand, aggregates and steel delivered across Bengaluru.

CementSand & AggregatesTMT BarsHardware
Shop nowGet a price listBengaluru · open 8 am–8 pm, all days

Frequently Asked Questions

What is the concrete slump test?

The concrete slump test measures how far a 300 mm high cone of fresh concrete settles once the mould is lifted. The drop in millimetres shows the consistency of the batch. In India it follows IS 1199 (Part 2):2018.

What is the purpose of slump test in concrete?

The purpose is to check the consistency, and so the workability, of fresh concrete before it is placed. It also catches batch-to-batch changes such as extra water. Ready-mixed concrete is accepted or rejected on slump at discharge.

What is a good slump for concrete?

A good slump is the one specified for the job, read as a true slump within the allowed tolerance. IS 456:2000 suggests 25–75 mm for lightly reinforced work and 50–100 mm for heavily reinforced sections. Pumped concrete is usually 75–100 mm.

What is the recommended slump for RCC work?

IS 456:2000 Clause 7.1 gives 25–75 mm for lightly reinforced slabs, beams and columns, and 50–100 mm for heavily reinforced members. If the concrete is pumped, 75–100 mm is typical. Always follow the slump in your structural drawings or mix design.

How is the concrete slump test performed?

Fill a damp slump cone in three equal layers and tamp each layer 25 times with a 16 mm rod. Strike off the top, lift the cone straight up in 5 ± 2 s and measure the drop to the highest point. Finish filling to lifting within 180 s.

What does the slump value indicate about concrete?

The slump value indicates how wet or stiff the fresh concrete is. A higher slump means a more fluid mix; a lower slump means a stiffer one. It does not indicate strength on its own, which depends on the water-cement ratio.

What are the different types of slump observed in the test?

The three types are true slump, shear slump and collapse slump. Only a true slump gives a valid reading. A shear or collapse means you take a fresh sample and repeat; two in a row make the test invalid.

What are the limitations of the concrete slump test?

The slump test only works for slumps of 10–210 mm, so it suits neither very stiff nor very fluid concrete. It cannot test self-compacting concrete, which needs a slump flow test. It also says little about pumpability or finishing.

Reviewed by

HomeRun Team

The HomeRun editorial team researches and writes our building guides.